Zinc Oxide (ZnO) Nanorods Green Synthesis by using Zinc Nitrate as precursor and Aloe Vera Leaves as reducing and stabilising agent via Biological Method.

  1. CHECK LIST
    Fresh leaves of Aloe Vera Leaves, Zinc Nitrate, Deionized Water, RB Flask, Dropper, Magnetic Stirrer with Temperature option, Filter Paper.

  2. STEP 1.
    Extract the gel from the Aloe Vera leaves to be used as Reducing and Capping agent for the synthesis.

  3. STEP 2.
    Take 30ml Aloe Vera gel and setup reflux at 80°C temperature.

  4. STEP 3.
    Take 3g Zinc Nitrate in 50ml water in another RB Flask.

  5. STEP 4.
    Add Zinc Nitrate solution (prepared in step-3) slowly in Aloe Vera gel (prepared in step-2) by dropper.

  6. STEP 5.
    After some time (~10min) White precipitation star appearing indicated the formation of Zinc Oxide Nanorods.

  7. STEP 6.
    Centrifuge the white precipitate at 5000 rpm for ~15 minutes to collect the powder.

  8. RESULTS
    UV-Vis absorbance of Zinc Oxide Nanorods obtained around 350nm. Diameter of Zinc Oxide Nanorods is around 40nm in size.

  9. NOTE: All the experiments should be done under the guidance of lab Incharge; and proper lab safety instructions.

2 Question, Ask New
thedarkobliteration says:

Instead of zinc nitrate can I use zinc chloride in the same procedure?

Help Team says:

You can use any precursor of Zinc but particles shape, size and morphology will change depending on the precursor and reducing agent

Ask Your Question